中国科技核心期刊
美国化学文摘社(CAS)数据库
美国EBSCO学术数据库
日本科学技术振兴机构数据库(JST)
An arsenic-bearing gold concentrate containing 52.80 g/t gold,6.31 % arsenic and 21.50 % sulfur is a typical refractory complex gold concentrate.The recovery of gold was not satisfactory by direct cyanidation and cyanidation after oxidation roasting and two-stage roasting pretreatment.Three-stage process (one-stage reduction roasting,two-stage acid leaching and three-stage oxidation roasting) was used in the experiment,and the experimental conditions were optimized.The results show that under optimal conditions,the gold leaching rate can be 93.60 % after reduction roasting-acid leaching-oxidation roasting-cyanidation treatment,6.80 percentage points higher than that by traditional two-stage roasting-cyanidation process,realizing the high value utilization of resources,providing technical basis for highly efficient recovery of arsenic-bearing gold concentrate.